Induction Hardening Pulleys
Views Send Enquiry
   Objective Heat cast iron pulleys to 1600ºF(871.1ºC) in order to achieve a hardness of 55 Rockwell C.
  Material Ductile Iron Pulleys measuring 3 1/2″(88.9mm) OD and 2″ (50.8mm) high.
  Temperature 1600ºF (871.1ºC)
  Frequency 164 kHz
  Equipment • Power of 10 kW induction heating system equipped with a remote workhead containing eight (8) capacitors totaling 0.66 μF
  • An induction heating coil designed and developed specifically for this application.
  Process A four turn helical coil is used to heat the cast iron pulley for 2 minutes and 45 seconds to reach the required 1600ºF (871.1ºC) Immediately following, the pulley is quenched in an agitated water bath to achieve the desired hardness.
  Results/Benefits Induction heating provides:
  • Increased production
  • Repeatable, non-contact and energy efficient heat
  • Precise heating
  
  
Related Content

Air Cooled clamp coil (half-open coil) for preheating gas pipeline

induction coating by air cooled clamp induction coil

Remove plastic coating from steel tubes by Induction Heating

Releasing Fixture by Induction Heating

U shape air cooled induction coil by UM-100C-HF for pipeline preheating

induction quenching with custom-design inductor

induction brazing diamond segment

induction brass soldering copper plate_2
Hot

induction hardening axle (shaft) by 100KW induction heater
induction quenching axle (shaft) by 160KW induction heater
induction hardening inner surface (inwall)
Induction Hardening Harvestor Combined Finger
Induction Hardening Harvestor Combined Blade
workpiece for induction hardening
induction hardening veterinary instrument
induction hardening surgical device

Newest Comment
No Comment
Post Comment